LEATHER
343

The process of manufacture is as follows: The hides are unhaired by short liming, painting with lime and sulphide, or sweating, and cleansed by scudding and washing, after which they are coloured in bark liquors, washed up through clean water, and hung up to dry partially. When in a sammied condition the goods are placed on a table and a thick layer of the tanning paste spread on the flesh side. The tanning paste varies with each manufacturer, but the following is the mixture originally used by Preller: 100 parts flour, 100 parts soft fat or horse tallow, 35 parts butter, 88 parts ox brains, 50 parts milk, 15 parts salt or saltpetre.

The hides are now rolled in bundles, placed in a warm drum and worked for 8 to 10 hours, after which they are removed and hung up until half dry, when the process is repeated. Thus they are tumbled 3 to 4 times, set out flesh and grain, rinsed through tepid water, set out, sammied, and curried by coating with glycerin, oil, tallow and degras. The table grease is now slicked off, and the goods are set out in grease, grained and dried.

Transparent Leather.—Transparent leather is a rather horny product, somewhat like raw hide, and has been used for stitching belts and picker bands. The goods to be dressed are limed, unhaired, very thoroughly delimed with acids, washed in water, scudded and clean-fleshed right to the veins; they are now stretched in frames, clean-fleshed with a moon knife, and brushed with warm water, when several coats of glycerin, to which has been added some antiseptic such as salicylic or picric acid, are applied; the goods are then dried out, and another coat is applied, and when semi-dry they are drummed in a mixture of glycerin, boracic acid, alum and salt, with the addition of a little bichromate of potash to stain them a yellow colour. After drumming for 2 to 3 hours they are removed, washed up, lightly set out, and stretched in frames to dry, when they are ready for cutting into convenient lengths for use.

Parchment.—A certain class of sheep skin known as Hampshires is generally used in the manufacture of this speciality. The skins as received are first very carefully washed to remove all dirt, dewooled, limed for 3 to 4 weeks, they are then cleanly fleshed, unhaired, rinsed up in water, and thickly split, the poorer hides being utilized for chamois; they are now re-split at the fatty strata so that all fat may be easily removed, and while the grains are dressed as skivers, the fleshes are tied in frames, watered with hot water, scraped and coated on both sides with a cream consisting of whiting, soda and water, after which they are dried out in a hot stove. In the drying the whiting mixture absorbs the grease from the skins; in fact, this method of degreasing is often employed in the manufacture of wool rugs. When dry, both sides of the skins are flooded to remove the whiting, and are then well rubbed over with a flat piece of pumice-stone, swilled, dried, re-pumiced, again swilled, and when sammied are rolled off with a wooden roller and dried out.

Tar and Peat Tanning.—Tar tanning was discovered by a French chemist named Philippi, who started with the idea that, if coal was a decomposition product of forests, it must still necessarily possess the tanning properties originally present in the trees. However far-fetched such an argument may seem, Philippi succeeded in producing a leather from wood and coal tar at a fairly cheap rate, the product being of excellent texture and strength, but rather below the average in the finish, which was inclined to be patchy, showing oily spots. His method consisted of impregnating the goods with refined tar and some organic acid, but the product does not seem to have taken any hold upon the market, and is not much heard of now.

Peat tanning was discovered by Payne, an English chemist, who was also the co-discoverer of the Payne-Pullman formaldehyde tanning process. His peat or humic acid tannage was patented by him about 1905, and is now worked on a commercial scale. The humic acid is first extracted from the peat by means of alkalis, and the hides are treated with this solution, the humic acid being afterwards precipitated in the hides by treatment with some stronger organic or mineral acid.

Dyeing, Staining and Finishing.—These operations are practised almost exclusively on the lighter leathers. Heavy leathers, except coloured and black harness and split hides for bag work, are not often dyed, and their finishing is generally considered to be part of the tannage. In light leathers a great business is done in buying up “crust” stock, i.e. rough tanned stock, and then dyeing and finishing to suit the needs and demands of the various markets. The carrying out of these operations is a distinct and separate business from tanning, although where possible the two businesses are carried on in the same works.

Whatever the goods are and whatever their ultimate finish, the first operation, upon receipt by the dyer of the crust stock, is sorting, an operation requiring much skill. The sorter must be familiar with the why and wherefore of all subsequent processes through which the leather must go, so as to judge of the suitability of the various qualities of leather for these processes, and to know where any flaws that may exist will be sufficiently suppressed or hidden to produce a saleable product, or will be rendered entirely unnoticeable. The points to be considered in the sorting are coarseness or fineness of texture, boldness or fineness of grain, colour, flaws including stains and scratches, substance, &c. Light-coloured and flawless goods are parcelled out for fine and delicate shades, those of darker hue and few flaws are parcelled out for the darker shades, such as maroons, greens (sage and olive), dark blues, &c., and those which are so badly stained as to be unsuitable for colours go for blacks. After sorting, the goods are soaked back to a limp condition by immersion in warm water, and are then horsed up to drip, having been given, perhaps, a preliminary slicking out.

Up to this point all goods are treated alike, but the subsequent processes now diverge according to the class of leather being treated and the finish required.

Persian goods for glacés, moroccos, &c., require special preparation for dyeing, being first re-tanned. As received, they are sorted and soaked as above, piled to samm, and shaved. Shaving consists of rendering the flesh side of the skins smooth by shaving off irregularities, the skin, which is supported on a rubber roller actuated by a foot lever, being pressed against a series of spiral blades set on a steel roller, which is caused to revolve rapidly. When shaved, the goods are stripped, washed up, soured, sweetened and re-tanned in sumach, washed up, and slicked out, and are then ready for dyeing.

There are three distinct methods of dyeing, with several minor modifications. Tray dyeing consists of immersing the goods, from 2 to 4 dozen at a time, in two separate piles, in the dye solution at 60° C, contained in a flat wooden tray about 5 ft. × 4 ft. × 1 ft., and keeping them constantly moving by continually turning them from one pile to the other. The disadvantages of this method are that the bath rapidly cools, thus dyeing rapidly at the beginning and slowly at the termination of the operation; hence a large excess of dye is wasted, much labour is required, and the shades obtained are not so level as those obtained by the other methods. But the goods are under observation the whole time, a very distinct advantage when matching shades, and a white flesh may be preserved. The paddle method of dyeing consists of paddling the goods in a large volume of liquor contained in a semi-circular wooden paddle for from half to three-quarters of an hour. The disadvantages are that the liquor cools fairly rapidly, more dye is wasted than in the tray method, and a white flesh cannot be preserved. But larger packs can be dyed at the one operation, the goods are under observation the whole time, and little labour is required.

The drum method of dyeing is perhaps best, a drum somewhat similar to that used by curriers being preferable. The goods are placed on the shelves inside the dry drum, the lid of which is then fastened on, and the machinery is started; when the drum is revolving at full speed, which should be about 12 to 15 revolutions per minute, the dye solution is added through the hollow axle, and the dyeing continued for half an hour, when, without stopping the drum, if desired, the goods may be fatliquored by running in the fatliquor through the hollow axle. The disadvantages are that the flesh is dyed and the goods cannot be seen. The advantages are that little labour is required, a large pack of skins may be treated, level shades are produced, heat is retained, almost complete exhaustion of the dye-bath is effected, and subsequent processes, such as fatliquoring, may be carried out without stopping the drum.

Of the great number of coal-tar dyes on the market comparatively few can be used in leather manufacture. The four chief classes are: (1) acid dyes; (2) basic or tannin dyes; (3) direct or cotton dyes; (4) mordant (alizarine) dyes.

Acid dyes are not so termed because they have acid characteristics; the name simply denotes that for the development of the full shade of colour it is necessary to add acid to the dye-bath. These dyes are generally sodium salts of sulphonic acids, and need the addition of an acid to free the dye, which is the sulphonic acid. Although theoretically any acid (stronger than the sulphonic acid present) will do for this purpose, it is found in practice that only sulphuric and formic acids may be employed, because others, such as acetic, lactic, &c., do not develop the full shade of colour. Acid sodium sulphate may also be successfully used.